Why bolts are hot-dip galvanized
Table of Contents
1. Hot-dip galvanizing (HDG)
What it is
Hot-dip galvanizing (often simply called galvanizing or hot-dip galvanizing) is a process in which pretreated steel parts are immersed in molten zinc. A zinc or zinc–iron alloy coating forms on the surface, producing a metallurgical bond between the coating and the steel.
For fasteners, hot-dip galvanized coatings are relatively thick — typically around 45–55 μm — which can be hard to tightly control. Because of their thickness and metallurgical bonding, HDG coatings offer excellent corrosion resistance and are widely used for structures such as steel tubular towers, poles, angle towers and photovoltaic mounting systems.
Advantages of hot-dip galvanized fasteners
- High reliability: The zinc coating metallurgically bonds to the steel and becomes part of the surface, so the coating is very durable.
- Complete coverage: The molten zinc reaches every part of the component — including recesses, sharp corners and blind holes — providing comprehensive protection.
- Low life-cycle cost: On a life-cycle basis, HDG rust protection is often less expensive than many paint systems.
- Time and labor saving: HDG is a technology-driven process that is faster and less labor-intensive than many manual coating methods (for example, painting). It reduces on-site coating work after installation and simplifies inspection (coating thickness can often be checked visually or with simple non-destructive gauges).
- Better atmospheric corrosion resistance compared with typical electroplated zinc layers because of the thicker, metallurgically bonded coating.
2. Sherardizing (powder/thermal diffusion zinc)
What it is
Sherardizing, often called thermal diffusion or powder zinc diffusion, produces a diffusion layer formed by a zinc–iron intermetallic (mainly the δ phase, FeZn₁₇). The δ phase contains about 7–11% Fe by mass, is dense and tough, and its corrosion resistance is comparable to that of hot-dip galvanizing. Typical hardness is around ~250 HV, giving good wear resistance.
The process uses zinc powder (and sometimes fillers such as alumina or refractory materials and ammonium chloride) under elevated temperatures so zinc diffuses into the steel surface.
Characteristics
- The diffusion layer is uniform and does not produce hydrogen embrittlement or dimensional distortion, making it especially suitable for nuts, bolts, small hardware, complex shapes, and powder-metallurgy parts.
- Disadvantages include harsher working conditions, greater environmental impact in some implementations, and difficulties with automating the process.
3. Mechanical plating (mechanical zinc)
What it is
Mechanical plating deposits zinc by using zinc powder, dispersants, accelerators and a liquid medium (usually water) together with a mechanical impact medium (e.g., glass beads). Parts are tumbled so that impacts embed zinc particles onto the surface, forming a zinc coating.
Characteristics
- Can be performed at room temperature and therefore avoids hydrogen embrittlement risks associated with some electroplating processes on high-strength steels.
- The process relies on mechanical impact to deposit zinc; it is distinct from electroplating and hot-dip methods.
- Drawbacks: coating thickness can be uneven, and the finish is usually less smooth and bright than an electroplated layer.
4. Electroplated zinc (electrogalvanizing / electroplating)
What it is
Electroplating zinc is the most common surface finish for many fasteners due to its attractive appearance and relatively low cost. Typical finishes include white zinc, blue-passivated, blue/white, and colored passivations.
Performance and notes
- Zinc electroplated layers are relatively pure and can be fine-grained and uniform; after chromate/passivation they can present white, iridescent or olive (military green) appearances for decorative and mild corrosion protection.
- Neutral salt spray performance for ordinary zinc electroplating is typically under 72 hours. Special sealing and passivation treatments can extend salt spray life to ~200 hours or more, but these treatments are significantly more expensive — often 5–8 times the cost of ordinary electroplating.
- Electroplating can introduce hydrogen embrittlement in high-strength fasteners unless proper baking/de-hydrogenation procedures are applied after plating. Electroplating has shorter acid/alkali resistance than thicker coatings and its environmental performance is generally worse than some newer alternatives unless wastewater is carefully treated.
- Common plating chemistries include cyanide zinc, zincate, chloride, and sulfate chemistries; choice depends on application, substrate and costs.
5. Dacromet (zinc-flake / Zn-Al flake coatings)
What it is
Dacromet (a trade name) refers to zinc–chromate or zinc-flake coatings commonly described as zinc-flake coatings or zinc-aluminum flake coatings. It is a non-electrolytic, paste-applied coating based on zinc flakes, aluminum flakes, chromates (or chromate-free passivations in modern formulations) and water.
Characteristics and advantages
- Very high corrosion resistance: Although the film thickness is relatively thin — typically 4–8 μm — Dacromet/zinc-flake systems can provide corrosion protection several times better than traditional electroplating or hot-dip in practice. For example, standard fasteners coated with Dacromet often pass 1200+ hours neutral salt spray without red rust.
- No hydrogen embrittlement: The process does not generate hydrogen, so it is suitable for load-bearing or high-strength fasteners.
- High temperature resistance: Dacromet coatings can withstand higher temperatures (often up to ~300 °C) compared with conventional zinc plating, which can fail above ~100 °C.
- Good adhesion and recoatability: The coating bonds well to the substrate and accepts additional organic coatings or paints if needed.
- Excellent coverage/penetration: The flake chemistry and application method allow coating of deep holes, inner surfaces and complex geometries that can be difficult to electroplate.
- Environment: Modern zinc-flake systems have lower environmental impact than some traditional chromate electroplating processes, and many formulations are designed to avoid hazardous byproducts.
| Process (common name) | Typical neutral salt-spray (NSS) performance (hours) | Typical coating thickness (μm) | Hydrogen-embrittlement (HE) risk | Typical applications |
|---|---|---|---|---|
| Hot-dip galvanizing (HDG) | ~720 → 2000+ (depends on thickness & service) | ~45–55 μm (typical for fasteners in many specs) | Low (metallurgical bond; HE uncommon) | Heavy structural steelwork, towers/poles, outdoor PV mounts, infrastructure |
| Sherardizing (thermal diffusion / powder zinc) | ~480 → 1000 (process & post-treatment dependent) | ~8–25 μm (diffusion layer) | Very low / none | Nuts, bolts, small/complex fasteners, powder-metallurgy parts where uniformity & no HE desired |
| Mechanical plating (mechanical zinc) | ~240 → 720 (varies with thickness & seal) | ~5–25 μm (can be non-uniform) | Low (room-temp process; avoids HE) | High-strength fasteners where HE must be avoided, retrofit work, small parts |
| Electroplated zinc (zinc electroplate + passivate) | ~24 → 200+ (plain finishes often <72 h; sealed/passivated systems can reach ~200 h or more) | ~5–15 μm (typical) | Higher (can cause HE on high-strength steels unless properly de-hydrogenated / baked) | General-purpose fasteners, decorative or light-duty outdoor use; economical option |
| Zinc-flake / Dacromet (Zn-flake) | ~480 → 1200+ (many systems commonly ≥1200 h with proper specs) | ~4–8 μm (thin, highly protective film) | None (non-electrolytic process) | High-performance fasteners (automotive, engineered assemblies), where thin, hydrogen-free, high corrosion resistance is required |
Summary — choosing a finish for fasteners
- Hot-dip galvanizing: Best for heavy structural components and outdoor systems where thick, long-lasting protection is required; expect larger thickness (45–55 μm) and possible dimensional/fit considerations.
- Sherardizing (thermal diffusion): Good for small fasteners and complex shapes where uniform diffusion coating and no hydrogen risk are priorities.
- Mechanical plating: Useful when room-temperature processing and hydrogen-embrittlement avoidance are important; finish is less bright and coating thickness can vary.
- Electroplated zinc: Low upfront cost and good appearance; requires hydrogen-embrittlement mitigation and has shorter corrosion life unless special sealing is used.
- Dacromet / zinc-flake: Excellent corrosion resistance in a thin, hydrogen-free coating; favored for high-performance fasteners in demanding environments.